AwlgripVarnish

Awlspar varnish: how to apply this classic tung oil yacht varnish

A one-component phenolic tung oil spar varnish: first coat 1:1 with T0016, 7–10 coats, P320–P400 sanding every 2–3 coats, 3–4 hours between coats.

  • 5 min read
  • Updated:

Awlspar is a classic, fast-drying, tung oil-based yacht varnish used to protect wooden caprails, hatches, ladders and interior/exterior "brightwork" from water and weather. Its amber tone deepens the colour of the wood.

Success with varnish lies not in the quality of a single coat but in the total film thickness. For exterior durability the application guide recommends at least 250 µm dry film over the peaks of the grain. That means 7–10 thin coats.

Awlspar varnish system cross-section
Awlspar is used on its own or under Awlbrite.

What does Awlspar do and where does it sit in the paint system?#

Awlspar can be used as a stand-alone system, or as the first 2–3 sealer coats in Awlgrip's "Ultimate Brightwork" system with two-component Awlbrite Clear applied over it.

Which surfaces and where is it used?#

  • Teak and mahogany caprails, hatches, ladders
  • Interior and exterior wooden details
  • Sealer coat under Awlbrite Clear

Surface preparation: the stage that decides the outcome#

New wood must be clean, dry, smooth and well seasoned. On oily woods (teak), excess oil is removed with teak cleaner or wood bleach and the residue completely washed off. Rough wood is sanded progressively with 60/80, 100/150, 220 and finally 320 grit. Old varnish in good condition is washed with Awlprep and dulled with 220–320 grit; varnish in poor condition is completely stripped.

Pre-application checklist0/4
Wood sanding sequence before varnishing
Progressive sanding.

Mix ratio, induction and pot life#

Awlspar is a one-component product. On new wood, the first coat for brushing is reduced 1:1 (100%) with T0016. For spray, the first coat is reduced 50–100% with T0180 and subsequent spray coats 25%. Subsequent brush coats usually need no reduction; if desired, up to 20% T0016 is added. The product is only stirred, never shaken.

Mixing and reduction values
CoatBrushSpray
First coat (new wood)T0016 100%T0180 50–100%
Subsequent coatsNot needed (≤ 20% T0016)T0180 25%

Application: step by step#

Use a natural-bristle brush, a foam or short-nap mohair roller, or spray. 50–75 µm wet, 25–37 µm dry film per coat. In a stand-alone system 7–10 coats are applied. Above 25 °C, 2–3 coats can be done in a day. Every 2–3 coats, after a 24-hour cure, sand with P320–P400.

Awlspar brush application
Thin and many coats.
  1. Preparation

    Cleaning and progressive sanding.

  2. First coat

    1:1 with T0016, penetrates the wood.

  3. Between coats

    Min. 3–4 h; max. 36 h without sanding.

  4. Intermediate sanding

    Every 2–3 coats, P320–P400 after 24 h.

  5. Total

    7–10 coats; ≥ 250 µm over the grain peaks.

Drying and recoat times#

At 25 °C and 50% humidity, Awlspar can be handled after about 24 hours.

Awlspar recoat times
Sand if past 36 hours.
Drying and recoat times
Condition (25 °C)Value
With itself, minimum3–4 h
Maximum without sanding36 h
Cure before sanding24 h
Before Awlbrite (Ultimate)≥ 72 h (7–10 days in cold weather)

Application conditions: temperature, humidity and dew point#

Best results are obtained at 18–32 °C. The surface must not be below 7 °C or above 41 °C, and curing must not be attempted below 7 °C. Avoid direct sunlight if possible.

Tips from the professionals#

  • Apply the first reduced coat liberally; let the wood absorb as much as it will, then wipe off the excess.
  • To control dust, wipe the surface and damp down the air with a damp cloth before varnishing.
  • Always finish the brush stroke in the same direction, along the grain.

Common mistakes#

Correct practice
  • First coat reduced 100%
  • 7–10 thin coats
  • P320–P400 every 2–3 coats
Common mistake
  • Shaken, causing bubbles
  • Few heavy coats
  • T0016 in urethane or epoxy

Health and safety#

Frequently asked questions#

How many coats of Awlspar are applied?

7–10 coats in a stand-alone system.

How is Awlspar thinned?

On new wood the first coat 1:1 with T0016; subsequent brush coats usually need none.

How long between coats of Awlspar?

At 25 °C at least 3–4 hours; max. 36 hours without sanding.

_Source: Awlgrip / AkzoNobel, Awlspar (M3131) technical data sheet (18.01.2019); Awlgrip Application Guide (22nd edition). The values on this page are compiled from documents published by the manufacturer and may change as the product evolves. Always check the product label, the current technical data sheet (TDS) and the safety data sheet (SDS) before application._